Rubberised Cork Sheet TG-7730 N
 
Grade TG-7730 N Specification Typical Result * Test Method
Binder.................................................... Synthetic
Rubber/Neoprene
Synthetic
Rubber/Neoprene
 
Cork Grain Size.....................................
Colour....................................................
0.5 to 1 mm
Natural
0.5 to 1mm
Natural
 
Physical Characteristics
Density.............Kg/m3..............................
Hardness, Shore A ..................................
Compressibility at400 PSI(%) ..................
Recovery after (%)..................................
Tensile Strength (Kg/cm2).......................

800-1040
65 – 85
20 ~ 35
80 min
1.72 min

950
71
26.02
85.38
2.37

ASTM F 1315
ASTM D 2240
ASTM F 36
ASTM F 36
ASTM F 152
Flexibility (Thickness X 3)
Original(F5).............................................
ASTM no.Oil,70hrs @ 100deg.C(F16)....
Oven aged ,70hrs @100deg.C(F16)......

No cracks
No cracks
No cracks

No Cracks
No cracks
No cracks

ASTM 147
Volume Change After Immersion
TransformerOil,70hrs @ 100degC(%)....
ASTM no.3 Oil,70 hrs @100deg C( %)...
Fuel A,22h RT............................
Thickness change (%)
IRM 903,70h @ 100 deg. C
Compression Set,Method A,
22h@70deg.C(max) (%).........................

- 10 to + 10
+ 5 to + 30
   0 + 15

   0 to +15

  50

1.85
24.77
2.18

12.01

46.27

ASTM F 147
ASTM F 146




ASTM D 395
*The results are based on typical samples tested in our lab. Due to the flexible and highly compressible nature of product, the results may vary at customers end.